Between leg tests, I wanted a small model of the 2.0 design that I could hold in my hand. It's 1/6 scale, about 113 × 60 × 70 mm, and uses about 48 g of gray PLA. I expected an easy side project. It took four full prints.

Joints that print assembled
My first plan was hinges made from pieces of 1.75 mm filament. Cutting and fitting that many tiny pins by hand didn't appeal to me, so I cancelled the test part as it started. The figure became print-in-place, which means it comes off the printer in one piece with its joints already together. Each joint has a small toothed wheel and two spring arms, so a leg clicks from one position to the next and holds there.
Small test joints came first. Hip settings were easy to choose, but one knee wouldn't move at all and another hurt my fingers. Those test levers reached only about 7 mm, while the real shank reaches 20.7 mm, so I printed a second set of knees with full-length levers. The best one was still a little too light, so the figure uses a slightly stiffer setting that I never tested on its own.
Four prints
| What changed | What happened | |
|---|---|---|
| 1 | Fast settings, slim tree supports | Body fine, all four legs spaghetti, stopped at about 4 hours |
| 2 | Much slower, stronger supports, nozzle lifts on every long move | Lower legs clean, pieces came loose at about 18 mm, stopped at about 3 hours |
| 3 | Medium speed, tiny break-away tabs across the joints | Pieces came loose at about 18 mm again, stopped at 100 minutes |
| One leg | A flat pad under the paw, bed held at 65 °C | Passed the trouble height, 44 minutes and about 4 g |
| 4 | Pads on all four paws, bed held at 65 °C | Finished in 6.5 hours, legs move and click |

Two wrong guesses
After print 1, I blamed speed and supports. Those changes did clean up the lower legs, so they may have helped, but the print still failed. Watching print 2's timelapse from the printer's camera, it looked as if a thigh had lifted off its support. That made sense, because each thigh starts as a loose island on top of a support, with nothing else holding it. So I added break-away tabs to tie the parts together.
Print 3 failed at the same height, even with the tabs and at a very different speed. That ruled out speed as the deciding factor. Then I took a close-up video from above, which I should have done much earlier. It showed clean, empty holes in the supports where the paws had been, and a whole shank lying flat on the plate. The paws were peeling off the bed.
Each paw touched the bed with only about 14 mm², and it had a tall, leaning leg above it. A normal slicer brim, a thin ring printed around a part to help it stick, wouldn't work well here because the supports crowd it out. So I added a 14 mm round pad to the model under each paw. Contact area went from about 55 mm² to 615 mm² in total. I still don't know exactly why the peeling starts at about 18 mm. My guess is that the plastic pulls harder as it shrinks once the thighs get wider.

Testing one leg first
This time I didn't jump straight to another full print. One leg printed past the failure height took 44 minutes. That test wasn't proof, since a single leg cools differently from a full plate, but it passed. The failed prints had already used about 8 hours.
Print 4 got through the trouble height cleanly. At about 44 mm, a small piece broke loose near the tip of the tail, which also starts as a loose island. It stayed a single piece and the rest was fine, so I let the print run. The hips and knees all click. The pads are hard to peel off, so they stay on as little feet.

Lessons
- Test the riskiest part first, and print it past the height where trouble is expected.
- Take a close-up photo or video before deciding what went wrong.
- Compare where each failure happens. Two prints failing at the same height at very different speeds said a lot.
- Check how much area touches the bed, especially under tall, leaning parts.
The slicing script now warns about small bed contact automatically, so the next print of this kind should catch the problem sooner.